비합금 구조용강
비합금 구조용강은 철에 수반되는 원소가 규정된 최소값을 초과하지 않는 모든 저탄소강을 포함한다. 항복강도, 성형성 및 용접성이 사용을 결정하는 주요 요인이다. 연하고, 유연하며, 인성이 있고, 신장성이 있지만 열처리로 경화할 수 없다.
| 강종 | 재료 번호 | P | S | C | Mn | Si | Al |
|---|---|---|---|---|---|---|---|
| SGP | — | max 0.04 | max 0.04 | — | — | — | — |
| STKM13B | — | max 0.04 | max 0.04 | max 0.25 | 0.3 - 0.9 | max 0.35 | — |
| SD300 | — | max 0.05 | max 0.05 | — | — | — | — |
| SGD2 | — | max 0.045 | max 0.045 | 0.1 - 0.15 | 0.3 - 0.6 | — | — |
| STKM14C | — | max 0.04 | max 0.04 | max 0.3 | 0.3 - 1 | max 0.35 | — |
| SD400W | — | — | — | — | — | — | — |
| STK500 | — | max 0.04 | max 0.04 | max 0.24 | 0.3 - 1.3 | max 0.35 | — |
| SNR400B | — | max 0.03 | max 0.03 | max 0.22 | 0.6 - 1.4 | max 0.35 | — |
| STKM16C | — | max 0.04 | max 0.04 | 0.35 - 0.45 | 0.4 - 1 | max 0.4 | — |
| SS590 | — | max 0.04 | max 0.04 | max 0.3 | max 1.6 | — | — |
| SM570 | — | max 0.035 | max 0.035 | max 0.18 | max 1.6 | max 0.55 | — |
| SD295A | — | max 0.05 | max 0.05 | — | — | — | — |
| STKM18B | — | max 0.04 | max 0.04 | max 0.18 | max 1.5 | max 0.55 | — |
| SPS490 | — | max 0.04 | max 0.04 | max 0.18 | max 1.5 | max 0.55 | — |
| STAM340G | — | max 0.035 | max 0.035 | max 0.2 | max 0.6 | max 0.35 | — |
| SFB3 | — | max 0.03 | max 0.035 | 0.15 - 0.3 | 0.4 - 1.2 | 0.15 - 0.5 | — |
| STC370 | — | max 0.04 | max 0.04 | max 0.25 | 0.3 - 0.9 | max 0.35 | — |
| SPPS380 | — | max 0.04 | max 0.04 | max 0.25 | 0.3 - 0.9 | max 0.35 | — |
| STAM500G | — | max 0.035 | max 0.035 | max 0.3 | 0.3 - 1 | max 0.35 | — |
| SFB7 | — | max 0.03 | max 0.035 | 0.4 - 0.6 | 0.5 - 1.2 | 0.15 - 0.5 | — |
| STC590A | — | max 0.04 | max 0.04 | max 0.25 | 0.3 - 0.9 | max 0.35 | — |
| SPPH490 | — | max 0.035 | max 0.035 | max 0.33 | 0.3 - 1.5 | 0.1 - 0.35 | — |
| STAM540H | — | max 0.035 | max 0.035 | max 0.3 | 0.3 - 1 | max 0.35 | — |
| SF490A | — | max 0.03 | max 0.035 | max 0.6 | 0.3 - 1.2 | 0.15 - 0.5 | — |
| SDR345 | — | max 0.03 | max 0.02 | max 0.27 | max 1.9 | max 0.55 | max 0.01 |
| STPG370 | — | max 0.04 | max 0.04 | max 0.25 | 0.3 - 0.9 | max 0.35 | — |
| SF590B | — | max 0.03 | max 0.035 | max 0.6 | 0.3 - 1.2 | 0.15 - 0.5 | — |
| SN490B | — | max 0.03 | max 0.015 | max 0.2 | max 1.65 | max 0.55 | — |
| STKN400W | — | max 0.03 | max 0.03 | max 0.25 | — | — | — |
| STW400 | — | max 0.04 | max 0.04 | max 0.25 | — | — | — |
| STPY400 | — | max 0.04 | max 0.04 | max 0.25 | — | — | — |
| STKM12A | — | max 0.04 | max 0.04 | max 0.2 | max 0.6 | max 0.35 | — |
| SD390 | — | max 0.04 | max 0.04 | max 0.29 | max 1.8 | max 0.55 | — |
| STS480 | — | max 0.035 | max 0.035 | max 0.33 | 0.3 - 1.5 | 0.1 - 0.35 | — |
| STKM13A | — | max 0.04 | max 0.04 | max 0.25 | 0.3 - 0.9 | max 0.35 | — |
| SR300 | — | max 0.05 | max 0.05 | — | — | — | — |
| SGD1 | — | max 0.045 | max 0.045 | max 0.1 | 0.3 - 0.6 | — | — |
| STKM14B | — | max 0.04 | max 0.04 | max 0.3 | 0.3 - 1 | max 0.35 | — |
| SD500 | — | max 0.05 | max 0.05 | — | — | — | — |
| STK490 | — | max 0.035 | max 0.035 | max 0.18 | max 1.65 | max 0.55 | — |
| SNR400A | — | max 0.05 | max 0.05 | max 0.24 | — | — | — |
| STKM16A | — | max 0.04 | max 0.04 | 0.35 - 0.45 | 0.4 - 1 | max 0.4 | — |
| SD700 | — | — | — | — | — | — | — |
| SM520C | — | max 0.035 | max 0.035 | max 0.2 | max 1.6 | max 0.55 | — |
| SR295 | — | max 0.05 | max 0.05 | — | — | — | — |
| STKM18A | — | max 0.04 | max 0.04 | max 0.18 | max 1.5 | max 0.55 | — |
| SPS500 | — | max 0.04 | max 0.04 | max 0.24 | 0.3 - 1.3 | max 0.35 | — |
| STAM290GB | — | max 0.035 | max 0.035 | max 0.12 | max 0.6 | max 0.35 | — |
| SFB2 | — | max 0.03 | max 0.035 | 0.1 - 0.25 | 0.3 - 1.2 | 0.15 - 0.5 | — |
| STKM19C | — | max 0.04 | max 0.04 | max 0.25 | max 1.5 | max 0.55 | — |
이 카테고리를 다루는 규격
32물성 범위
21| 물성 | 단위 | 하한 | 상한 | 강종 수 |
|---|---|---|---|---|
| ReH | N/mm² | 120 | 550 | 45 |
| Rm | N/mm² | 255 | 1050 | 182 |
| A80 | % | 4 | 32 | 17 |
| Re | N/mm² | 165 | 700 | 145 |
| A | % | 5 | 41 | 151 |
| A5 | % | 7 | 36 | 29 |
| Z | % | 18 | 68 | 23 |
| aK | J/cm² | 29 | 98 | 4 |
| KCU | kJ/m² | 240 | 780 | 6 |
| HB | — | 90 | 255 | 28 |
| HV | — | 100 | 105 | 3 |
| rho | g/cm³ | 7.582 | 7.871 | 319 |
| E | GPa | 141 | 213 | 7 |
| alpha | 10^-6/K | 11 | 15.6 | 6 |
| lambda | W/(m·K) | 27 | 76 | 6 |
| cp | J/(kg·K) | 466 | 875 | 6 |
| rho_el | nΩ·m | 140 | 1135 | 5 |
| Ac1 | °C | 720 | 745 | 13 |
| Ac3 | °C | 770 | 880 | 13 |
| Ar3 | °C | 755 | 854 | 12 |
| Ar1 | °C | 677 | 700 | 13 |
이 카테고리에서 값이 기록된 319 강종를 기준으로 산출.
화학 성분 범위
15| 물성 | 단위 | 하한 | 상한 | 강종 수 |
|---|---|---|---|---|
| B | % | 0.0008 | 0.005 | 1 |
| C | % | 0.004 | 0.6 | 318 |
| N | % | 0.0012 | 0.1 | 85 |
| Al | % | 0.01 | 0.06 | 38 |
| Si | % | 0.03 | 4.5 | 217 |
| P | % | 0.01 | 0.12 | 336 |
| S | % | 0.015 | 0.08 | 336 |
| Ti | % | 0.03 | 0.3 | 26 |
| V | % | 0.02 | 0.2 | 11 |
| Cr | % | 0.12 | 0.5 | 18 |
| Mn | % | 0.03 | 1.9 | 283 |
| Ni | % | 0.12 | 0.3 | 17 |
| Cu | % | 0.03 | 0.55 | 42 |
| Nb | % | 0.01 | 0.08 | 12 |
| Mo | % | 0.05 | 0.35 | 14 |
이 카테고리에서 값이 기록된 336 강종를 기준으로 산출.
열처리
3| 공정 | 하한온도(°C) | 상한온도(°C) | 강종 수 |
|---|---|---|---|
| normalizing | — | — | 4 |
| annealing | — | — | 3 |
| tempering | — | — | 1 |