SWR-7
SWR-7 is a designation in JIS for the material held under material number 1.0601, also listed as C60. It is a material in the category Quenched and tempered steels. We list 92 designations recorded for this grade, in the standards DIN / EN, UNS, AISI / SAE, BS, AFNOR, UNE, ISO, JIS, GB, GOST, UNI, SS, ČSN, COPANT, STN, PN, SRPS, HRN, MSZ, AS / NZS, STAS, BDS, ÖNORM, NBN, SNV and KS.
If you came for one of these
The most-used names for this grade.About Quenched and tempered steels
Quenched and tempered steels are heat-treated steels designed to combine high strength with useful toughness and ductility. They are used for heavily loaded components such as shafts, gears, fasteners and structural machine parts where resistance to mechanical stress is required.
This describes the material class as a whole. Always confirm the individual grade against the standard before ordering.
Also known as
92 designations · 26 standards · nothing hidden- S58CIndicative
- S60C-CSPIndicative
- S65C-CSPIndicative
- SWR-7Indicative
Every designation on file is listed — no truncation, no “+ n more”. Each one is itself a route that leads back here.
Chemical composition
8 elements on file · weight %What this alloy is
Logarithmic scale, 0.01 % to 100 % — every value here compares directly, decade by decade.
| Element | % by weight |
|---|---|
0.57–0.65 | |
≤ 0.4 | |
0.6–0.9 | |
0.045 | |
0.045 | |
≤ 0.4 | |
≤ 0.1 | |
≤ 0.4 |
The scale is logarithmic, not the element’s raw share of the alloy — the only honest way to fit 0.01 % and 100 % in one picture, and it means every value here can be compared with every other.
| Element | As publishedsource text, verbatim | Min% by weight | Max% by weight | Bound |
|---|---|---|---|---|
| C | 0,57-0,65 | 0.570 | 0.650 | Range |
| Si | ≤0,40 | — | 0.400 | Max |
| P | 0,045 | 0.045 | 0.045 | Exact |
| S | 0,045 | 0.045 | 0.045 | Exact |
| Cr | ≤0,40 | — | 0.400 | Max |
| Mn | 0,60-0,90 | 0.600 | 0.900 | Range |
| Ni | ≤0,40 | — | 0.400 | Max |
| Mo | ≤0,10 | — | 0.100 | Max |
- (Cr + Mo + Ni) ≤ 0,63
- (Cr + Mo + Ni) ≤ 0,63
- (Cr + Mo + Ni) ≤ 0,63
The published column is the source string byte-for-byte, decimal comma and all; Min and Max are the parsed bounds. Elements not listed have no value on file — they are omitted, never inferred.
Predicted transformation temperatures
This grade's composition falls outside the published model's validated range (a low-alloy composition window), so no transformation temperature is predicted here.
Physical & mechanical properties
An absent property means we hold no value for it — it is left out rather than estimated, interpolated from a neighbouring grade, or filled from a handbook. It does not mean the property is undefined for the material.
Properties by condition
8 conditions · 39 valuessplav| Delivery state | RmN/mm² | A5% | HB |
|---|---|---|---|
| Band cold-worked , GOST 2283-79 | 740 – 1180 | — | — |
| Band annealed , GOST 2283-79 | 640 – 740 | 10 – 15 | — |
| (without heat treatment) , GOST 14959 | — | — | 285 |
| (heat treatment) , Rolled stock GOST 14959-79 | — | — | 241 |
| (normalize) , Sheet trick GOST 1577-93 | — | — | 269 |
| (annealing) , Sheet trick GOST 1577-93 | — | — | 229 |
steelnumber| Thicknessmm | RmN/mm² | A% |
|---|---|---|
| ≤ 16 | 710 | 10 |
| 16 – 100 | 670 | 11 |
| 100 – 250 | 650 | 11 |
| 250 – 500 | 630 | — |
| 500 – 1000 | 620 | — |
steelnumber| Thicknessmm | RmN/mm² | A% |
|---|---|---|
| 5 – 10 | 800 – 1150 | 5 |
| 10 – 16 | 780 – 1130 | 5 |
| 16 – 40 | 730 – 1100 | 6 |
splav| Heat-treated condition | RmN/mm² | ReN/mm² | A5% | Z% |
|---|---|---|---|---|
| Rolled stock, GOST 14959-79 | 980 | 785 | 8 | 30 |
steelnumber| Delivery state | HB |
|---|---|
| Treated to improve shearability | 255 |
steelnumber| Delivery state | HB |
|---|---|
| Soft annealed | 241 |
steelnumber| Delivery state | HB |
|---|---|
| As rolled and turned | 198 – 278 |
splav| Temperature°C | Densityg/cm³ | Elastic modulusGPa | Thermal expansion coefficient10^-6/K | Specific heat capacityJ/(kg·K) |
|---|---|---|---|---|
| 20 | 7.81 | 204 | — | — |
| 100 | — | — | 11.6 | 483 |
| 200 | — | — | 11.9 | 487 |
| 300 | — | — | 12.9 | — |
| 400 | — | — | 13.8 | 529 |
| 600 | — | — | 14.6 | 575 |
Every figure holds only for the condition on its own row. Values are never merged across conditions or across sources, never averaged, and never interpolated between two rows. An em dash means no value on file — never zero. Figures are converted to the unit in the column header; the source’s own wording is kept and shown where the two differ.
Similar grades — and why
Selection rule, stated so you can disagree with it: same number class 1.0, a shared category, and a published range for Mn / Si that overlaps this grade’s. These are neighbours in composition space — they are not equivalents, and none is claimed to be interchangeable with this grade.
Mn 0,60-0,90 · Si ≤0,40
- ΔMn 0.00
- ΔSi 0.00
- 101 designations
Mn 0,60-0,90 · Si ≤0,40
- ΔMn 0.00
- ΔSi 0.00
- 25 designations
Mn 0,40-1,10 · Si ≤0,35
- ΔMn 0.00
- ΔSi 0.03
- 10 designations
Mn 0,50-0,80 · Si 0,10-0,30
- ΔMn 0.10
- ΔSi 0.00
- 8 designations
Mn 0,50-0,80 · Si ≤0,40
- ΔMn 0.10
- ΔSi 0.00
- 123 designations
Mn 0,50-0,80 · Si ≤0,40
- ΔMn 0.10
- ΔSi 0.00
- 2 designations